Learn

  • Physics
  • Chemistry
  • Mathematics
  • Biology
  • Python Programming
  • Statistics & Data Science
  • Computer Science
  • Space Science and Astronomy
  • Classes
  • Groups

Practice

  • Problems
  • Quizzes
  • Mock Tests
  • Prepare for an Exam
  • Question Sets
  • Exams
  • Certificates
  • Python Labs
  • AI Practice Generator
  • Student-Created Tests

Community

  • Discussions
  • Resources
  • Notes
  • Glossary
  • Blog

Account

  • Log in
© 2026 senLearn. All rights reserved.HelpFor SchoolsAboutContactPrivacy PolicyTerms of UseRefund Policy
Electrolysis, Refining and the Extraction of Four Metals
  1. 1Electrochemical extraction: aluminium, displacement and chlorine
  2. 2Refining a crude metal
  3. 3Iron, copper and zinc from ore to metal, with uses and recycling
  1. Chemistry
  2. /Electrolysis, Refining and the Extraction of Four Metals
  3. /Iron, copper and zinc from ore to metal, with uses and recycling

Course 35.3·Lesson 3 of 3

Iron, copper and zinc from ore to metal, with uses and recycling

A blast furnace runs for years without stopping. Copper ore turns into a bubbly metal called blister copper. Zinc is made in two quite different ways. This lesson follows iron, copper and zinc from their ores to the metal, and ends with what the metals are used for and why recycling matters.

about 25 min1 simulation1 practice question
Lesson 3 of 3Show all lessonsHide
Electrolysis, Refining and the Extraction of Four Metals
  1. 1Electrochemical extraction: aluminium, displacement and chlorine
  2. 2Refining a crude metal
  3. 3

Try the code and the simulations beside the lesson.

Iron: the blast furnace

A blast furnace drawn in section, tall and narrow. At the top, ore, coke and limestone go in, and waste gases leave. In the upper zone, about 500 to 800 K, carbon monoxide reduces iron(III) oxide to iron(II, III) oxide and iron(II) oxide. In the middle zone, about 900 to 1500 K, carbon dioxide meets coke and turns into carbon monoxide, and iron(II) oxide is reduced to iron; limestone gives lime that joins silica as slag. Near the bottom, hot air is blown in through tuyeres and coke burns, reaching about 2000 K. Molten slag floats on molten iron at the bottom, and each is tapped off.

The charge. Haematite (after calcination), coke and limestone go in at the top. Hot air is blown in near the bottom through pipes called tuyeres.

The bottom: about 2000 K. Coke burns in the hot air. C + O2 → CO2\text{C}\ +\ \text{O}_{2}\ \rightarrow \ \text{CO}_{2}C + O2​ → CO2​ This gives the heat.

The middle: 900 to 1500 K. Carbon dioxide meets more coke. CO2 + C → 2CO\text{CO}_{2}\ +\ \text{C}\ \rightarrow \ 2\text{CO}CO2​ + C → 2CO Iron(II) oxide is reduced. FeO + CO → Fe + CO2\text{FeO}\ +\ \text{CO}\ \rightarrow \ \text{Fe}\ +\ \text{CO}_{2}FeO + CO → Fe + CO2​ and FeO + C → Fe + CO\text{FeO}\ +\ \text{C}\ \rightarrow \ \text{Fe}\ +\ \text{CO}FeO + C → Fe + CO Limestone breaks up, CaCO3 → CaO + CO2\text{CaCO}_{3}\ \rightarrow \ \text{CaO}\ +\ \text{CO}_{2}CaCO3​ → CaO + CO2​, and lime joins the silica as slag, CaO + SiO2 → CaSiO3\text{CaO}\ +\ \text{SiO}_{2}\ \rightarrow \ \text{CaSiO}_{3}CaO + SiO2​ → CaSiO3​.

The top: 500 to 800 K. Carbon monoxide reduces the higher oxides:

3Fe2O3 + CO → 2Fe3O4 + CO23\text{Fe}_{2}\text{O}_{3}\ +\ \text{CO}\ \rightarrow \ 2\text{Fe}_{3}\text{O}_{4}\ +\ \text{CO}_{2}3Fe2​O3​ + CO → 2Fe3​O4​ + CO2​, Fe3O4 + 4CO → 3Fe + 4CO2\text{Fe}_{3}\text{O}_{4}\ +\ 4\text{CO}\ \rightarrow \ 3\text{Fe}\ +\ 4\text{CO}_{2}Fe3​O4​ + 4CO → 3Fe + 4CO2​, Fe2O3 + CO → 2FeO + CO2\text{Fe}_{2}\text{O}_{3}\ +\ \text{CO}\ \rightarrow \ 2\text{FeO}\ +\ \text{CO}_{2}Fe2​O3​ + CO → 2FeO + CO2​

Molten iron sinks to the bottom. The lighter slag floats on it and protects it from the air. Both are tapped off.

Kinds of iron.

  • Pig iron, from the furnace, holds about 4 % carbon and small amounts of silicon, manganese, sulphur and phosphorus. It is hard and brittle.
  • Cast iron, made by melting pig iron with scrap iron and coke in a hot-air blast, holds about 3 % carbon. It is very hard and brittle.
  • Wrought iron is the purest commercial iron. It is made from cast iron in a reverberatory furnace lined with haematite, which oxidises the carbon: Fe2O3 + 3C → 2Fe + 3CO\text{Fe}_{2}\text{O}_{3}\ +\ 3\text{C}\ \rightarrow \ 2\text{Fe}\ +\ 3\text{CO}Fe2​O3​ + 3C → 2Fe + 3CO. Limestone is added as a flux, and the iron is taken out and rolled.
  • Steel holds 0.1 to 1.5 % carbon. Today most steel is made by blowing pure oxygen through molten pig iron, which burns out most of the carbon, silicon and phosphorus.

Set 75 % haematite and 8 % silica. The furnace needs nearly two tonnes of ore and more than 250 kg of limestone for each tonne of iron. A richer ore saves on both.

Copper: from pyrites to blister copper

  1. Concentration of copper pyrites by froth flotation.
  2. Roasting in a reverberatory furnace. Part of the sulphide turns into oxides, and sulphur dioxide leaves.
  3. Smelting with silica. Iron(II) oxide becomes slag, FeO + SiO2 → FeSiO3\text{FeO}\ +\ \text{SiO}_{2}\ \rightarrow \ \text{FeSiO}_{3}FeO + SiO2​ → FeSiO3​. Any copper oxide is turned back into sulphide by iron(II) sulphide, Cu2O + FeS → Cu2S + FeO\text{Cu}_{2}\text{O}\ +\ \text{FeS}\ \rightarrow \ \text{Cu}_{2}\text{S}\ +\ \text{FeO}Cu2​O + FeS → Cu2​S + FeO, because copper holds sulphur more strongly than iron does. The molten copper matte, Cu2S\text{Cu}_{2}\text{S}Cu2​S with some FeS\text{FeS}FeS, is run off.
  4. The converter. Air is blown through the molten matte with silica. The rest of the iron goes first: 2FeS + 3O2 → 2FeO + 2SO22\text{FeS}\ +\ 3\text{O}_{2}\ \rightarrow \ 2\text{FeO}\ +\ 2\text{SO}_{2}2FeS + 3O2​ → 2FeO + 2SO2​ and FeO + SiO2 → FeSiO3\text{FeO}\ +\ \text{SiO}_{2}\ \rightarrow \ \text{FeSiO}_{3}FeO + SiO2​ → FeSiO3​. Then copper(I) sulphide is partly oxidised, 2Cu2S + 3O2 → 2Cu2O + 2SO22\text{Cu}_{2}\text{S}\ +\ 3\text{O}_{2}\ \rightarrow \ 2\text{Cu}_{2}\text{O}\ +\ 2\text{SO}_{2}2Cu2​S + 3O2​ → 2Cu2​O + 2SO2​, and the self-reduction gives copper: 2Cu2O + Cu2S → 6Cu + SO22\text{Cu}_{2}\text{O}\ +\ \text{Cu}_{2}\text{S}\ \rightarrow \ 6\text{Cu}\ +\ \text{SO}_{2}2Cu2​O + Cu2​S → 6Cu + SO2​.

The copper that comes out has a blistered surface, because sulphur dioxide escapes as it sets. It is called blister copper, about 98 to 99 % pure. It is poled and then refined by electrolysis.

Copper from low-grade ores and scrap is won by leaching and displacement, or by electrolysis of the leach liquor.

Zinc: two routes

  1. The retort. Zinc blende is concentrated by flotation and roasted to zinc oxide. The oxide is mixed with coke and heated in a fireclay retort near 1673 K. ZnO + C → Zn + CO\text{ZnO}\ +\ \text{C}\ \rightarrow \ \text{Zn}\ +\ \text{CO}ZnO + C → Zn + CO Zinc distils off and is condensed.
  2. Electrolysis. Most zinc is now made this way. The roasted oxide is dissolved in dilute sulphuric acid, the solution is purified, and zinc is plated on aluminium cathodes. Zn2+ + 2e− → Zn\text{Zn}^{2+}\ +\ 2\text{e}^{-}\ \rightarrow \ \text{Zn}Zn2+ + 2e− → Zn Oxygen comes off at the lead anodes, and the sulphuric acid is used again. The zinc is about 99.95 % pure.

Uses of the four metals

  • Aluminium: foil for food, cooking utensils, overhead power cables, window frames, alloys for aircraft and cars, aluminium powder in paints and in the thermite process.
  • Iron: cast iron for stoves, pipes and machine bases; wrought iron for chains, anchors, bolts and wire; steel for buildings, bridges and vehicles. Nickel steel is used for cables and car parts, chrome steel for cutting tools, and stainless steel for utensils, cycles and surgical tools.
  • Copper: electric wires, water pipes, and alloys: brass with zinc, bronze with tin, and the copper and nickel alloys of coins.
  • Zinc: galvanising iron, dry cells, brass, die-cast parts, and zinc dust as a reducing agent.

Recycling

Making aluminium from bauxite needs a huge amount of electricity, about 14 kWh for each kilogram in the cell alone. Melting scrap aluminium needs only about 5 % of that energy, because the Al to O bonds do not have to be broken again. Recycling also saves the bauxite, the red mud and the carbon dioxide from the anodes. Steel and copper are recycled widely for the same reasons. A drink can may be back on a shelf within weeks.

Practise with new numbers

Try it in Python

The program works out the ore, limestone, slag and carbon for one tonne of iron.

Read it first. Predict how the limestone changes if the ore is richer in haematite but holds the same share of silica. Then run it.

1. Change ore_fe2o3 to 0.90. Which numbers change?

2. Real furnaces burn about 450 kg of coke for each tonne of iron. Why is that more than the carbon the program gives?

Common mistakes

  • Putting the reduction of haematite in the hottest zone. It happens near the top, by carbon monoxide.
  • Calling pig iron the purest iron. Wrought iron is the purest commercial form.
  • Skipping the silica in copper smelting. Without it, iron would stay with the copper.
  • Thinking blister copper is pure. It still needs poling and electrolysis.

Remember these

  • Blast furnace: top 500 to 800 K (CO reduces Fe2O3\text{Fe}_{2}\text{O}_{3}Fe2​O3​), middle 900 to 1500 K (FeO reduced, slag forms), bottom about 2000 K (coke burns).
  • Pig iron about 4 % C; cast iron about 3 %; wrought iron purest; steel 0.1 to 1.5 %.
  • Copper: flotation, roasting, matte, converter, blister copper, electrolysis.
  • Zinc: retort near 1673 K, or electrolysis of zinc sulphate.
  • Recycling aluminium needs about 5 % of the energy.

References

  • NCERT Chemistry Part I for Class 12 (2007 edition), Unit 6, the sections on the extraction of iron, copper and zinc and on the uses of metals.
  • Greenwood and Earnshaw, Chemistry of the Elements, the chapters on iron and on copper.

Check yourself

Try each one on your own first. If you are stuck, open a hint. Then check with Show the answer.

  1. What is the job of limestone in a blast furnace?
  1. Why is the copper from the converter called blister copper?
  1. Write the self-reduction step in the converter.
  1. Why does recycling aluminium save so much energy?

Enroll free in Electrolysis, Refining and the Extraction of Four Metals

Every lesson is open to read. Enrolling also lets you:

  • Mark lessons done and carry on where you stopped.
  • Take the tests of this lesson and its course.
  • Count the course towards the certificate for its chapter.
No payment. You can leave at any time.

Problems (3)

A blast furnace makes one tonne of pig iron that is 95 % iron and 4.0 % carbon by mass…Advanced · High School (11–12) · by StemPy Lab
A copper smelter treats 10.0 t of concentrate that holds 25.0 % copper pyrites, CuFeS₂, and the…Hard · High School (11–12) · by StemPy Lab
A zinc plant plates zinc from purified zinc sulphate solution onto aluminium cathodes…
That was the last lessonBack to the course: take the test
← Electrolysis, Refining and the Extraction of Four Metals
← Refining a crude metalNext →

Discussion (0)

Log in to join the discussion.

Loading…

1 Python program
4 questions to check yourself

This lesson is free to read. Enroll free to keep your place and take the tests.

Iron, copper and zinc from ore to metal, with uses and recycling
Advanced · High School (11–12) · by StemPy Lab

Question Sets (1)

Refining and Extraction: Practice Questions10 questions · by StemPy Lab

Notes (1)

Electrolysis, Refining and Extraction: Quick RevisionNote · by StemPy Lab